Concrete is a material that carries tension poorly, so cracks appear in reinforced concrete structures. In an ordinary structure this is normal; in a tank that has to hold liquid and gas, a crack can become a leakage path. The question is therefore not "are there cracks" but "what is their width, are they through-cracks and do they change".
Where cracks come from
The most common causes are:
- setting and drying shrinkage: the concrete shrinks, and the reinforcement bars and previously built parts (for example the base slab) restrain this deformation,
- thermal stresses: heat of hydration in thick walls and later temperature differences between the warm interior and the cold exterior,
- uneven settlement of the ground,
- loads from liquid pressure, mixers and the roof,
- workmanship errors: too little cover, improper curing, construction joints.
A heated digester is particularly susceptible to thermal stresses, because the wall constantly has a different temperature on each side.
Cracks and tightness in EN 1992-3
Eurocode 2 Part 3 introduces tightness classes (from 0 to 3). Class 0 allows some leakage, higher classes limit it depending on the medium. The limiting crack width in a class that allows limited leakage is determined depending on the ratio of the height of the liquid column to the wall thickness; the values lie in the range of about 0.05–0.2 mm, and the exact figures follow from the standard and the national annex, so we quote them as an order of magnitude, not as a requirement. For gas, it is assessed separately whether a crack can be a through-crack. In practice the designer assumes that some narrow cracks close by themselves thanks to the precipitation of calcium carbonate and the swelling of the cement paste.
When a crack is acceptable
A crack usually does not require intervention when:
- it does not leak and is not a through-crack,
- its width is within the limit set by the design,
- it does not grow over time (confirmed by measurement or a plaster tell-tale),
- it is not in a zone exposed to chemical attack or to reinforcement corrosion.
A crack should be described, measured with a graduated magnifier and marked on a drawing, so that its change can be assessed later.
When intervention is needed
Intervention is necessary when a crack leaks, is wider than the design limit, opens and closes under the influence of temperature or load, or is in the gas zone, where it leads to acidic condensate reaching the reinforcement. Cracks in the base slab and at the joint with the wall are particularly troublesome, because they are hard to observe.
Repair methods
The choice depends on whether the crack is active:
- Epoxy resin injection – restores the structural continuity of a passive crack; requires a dry or suitably prepared substrate.
- Polyurethane injection – flexible, suitable for sealing damp and slightly moving cracks.
- Cement or mortar injection – for wider gaps of a non-structural nature.
- Surface sealing with a flexible material or tape – for moving cracks, where a rigid filler would crack again.
- A coating or lining bridging cracks over the whole surface – when there are many cracks.
The PN-EN 1504 series organises the principles of concrete repair and protection, including the principles of product selection and quality control. Injection repairs are carried out after the tank has been emptied and cleaned.
Prevention
The risk is reduced by: a proper concrete recipe (low w/c, control of the heat of hydration), minimum reinforcement limiting crack opening, moist curing, fewer construction joints and joint strips, and an even substrate. The way of start-up also matters: rapid heating of an empty tank increases thermal stresses, so heating should rise gradually.
Monitoring
After acceptance it is worth keeping a crack register: location, width, date of measurement, photograph. Repeated every few months in the first year and then once a year, it makes it possible to distinguish stabilised cracks from active ones. It is a simple task that saves costly repairs at an unexpected moment.
What to look out for
In the as-built documentation it is worth keeping photographs and a description of the cracks visible after the water test. They provide a reference point without which it is hard to judge whether a crack appeared after acceptance or was there from the start. Clear records also make it easier to discuss responsibility for repair during the warranty period and protect both parties from a dispute.
Summary
Cracks in tank concrete are part of the life of the structure. What matters is their width, whether they pass through and whether they move, and compliance with a design based on EN 1992-3. The repair method is chosen after the cause has been assessed, not the other way round.